wood, pine (#773)
ID-number | #773 |
---|---|
Material | wood, pine |
Classification | ECN Phyllis classification ▸ untreated wood ▸ fir/pine/spruce ▸ wood, pine |
NTA 8003 classification ▸ [100] hout ▸ [110] vers hout ▸ [130] naaldhout ▸ [131] naaldhout | |
Submitter organisation | ECN (Netherlands) |
Literature | R. Zevenhoven et.al.: Pressurized gasification properties of fossil fuels, bio-fuels and wastes. In: Finnish-Swedish Flame Days 1996, September 3-4, Naantali, Finland, pp. 1-31, Abo Akademi University, Combustion Chemistry Research Group, Turku/Abo. |
Values
Property | Unit | Value | Std dev | Det lim | Lab | Date | Method | Remarks | ||||||||||||
---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
ar | dry | daf | ||||||||||||||||||
Main biomass properties |
||||||||||||||||||||
Proximate analysis |
||||||||||||||||||||
Moisture content | wt% | 6.20 | ||||||||||||||||||
Ash content | wt% | 0.47 | 0.50 | |||||||||||||||||
Volatile matter | wt% | 85.78 | 91.45 | 91.91 | ||||||||||||||||
Fixed carbon | wt% | 7.55 | 8.05 | 8.09 | Calculated | |||||||||||||||
Ultimate analysis (macroelements) |
||||||||||||||||||||
Carbon | wt% | 45.87 | 48.90 | 49.15 | Measured | |||||||||||||||
Hydrogen | wt% | 5.63 | 6.00 | 6.03 | Measured | |||||||||||||||
Oxygen | wt% | 41.08 | 43.80 | 44.02 | Measured | |||||||||||||||
Nitrogen | wt% | 0.19 | 0.20 | 0.20 | Measured | |||||||||||||||
Sulphur | wt% | 0.06 | 0.06 | 0.06 | Measured | |||||||||||||||
Total (with halides) | wt% | 99.49 | 99.46 | 99.46 | Calculated | |||||||||||||||
Heating value |
||||||||||||||||||||
Net calorific value (LHV) | MJ/kg | 16.54 | 17.80 | 17.89 | ||||||||||||||||
Gross calorific value (HHV) | MJ/kg | 17.92 | 19.11 | 19.21 | ||||||||||||||||
HHVMilne | MJ/kg | 18.13 | 19.32 | 19.42 | Calculated |