bark, Premna bengalensis (#2055)
ID-number | #2055 |
---|---|
Material | bark, Premna bengalensis |
Classification | ECN Phyllis classification ▸ untreated wood ▸ bark |
NTA 8003 classification ▸ [100] hout ▸ [110] vers hout ▸ [112] schors | |
Submitter organisation | ECN (Netherlands) |
Submission date | 2001-04-04 |
Remarks | subtropical tree from north-east India; also data on trunk, twigs and leaves (ID 2054, 2056, 2057) |
Literature | Kataki,R; Konwer,D: Fuelwood characteristics of some indigenous woody species of north-east India; Biomass & Bioenergy 20 (2001) 17-23 |
Values
Property | Unit | Value | Std dev | Det lim | Lab | Date | Method | Remarks | ||||||||||||
---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
ar | dry | daf | ||||||||||||||||||
Main biomass properties |
||||||||||||||||||||
Proximate analysis |
||||||||||||||||||||
Moisture content | wt% | 71.20 | ||||||||||||||||||
Ash content | wt% | 2.68 | 9.29 | |||||||||||||||||
Ultimate analysis (macroelements) |
||||||||||||||||||||
Total (with halides) | wt% | 73.88 | 9.29 | 0.00 | Calculated | |||||||||||||||
Heating value |
||||||||||||||||||||
Gross calorific value (HHV) | MJ/kg | 4.62 | 16.04 | 17.68 | ||||||||||||||||
Biochemical analysis |
||||||||||||||||||||
Cellulose, hemicellulose, lignin |
||||||||||||||||||||
Cellulose | wt% (dry) | 18.06 | Measured | |||||||||||||||||
Hemicellulose | wt% (dry) | 33.73 | Measured | |||||||||||||||||
Lignin | wt% (dry) | 19.55 | Measured | |||||||||||||||||
Other |
||||||||||||||||||||
Extractives EtOH/toluene | wt% (dry) | 2.61 | Measured | |||||||||||||||||
Extractives hot water | wt% (dry) | 13.95 | Measured | |||||||||||||||||
Total ash + biochemical | wt% (dry) | 97.19 | Calculated |